2015年6月8日星期一

Plastic product deformation analysis method

One. Deformation causes:
1, the shape of the article, particularly molding shrinkage rates with the relationship between the residual stress caused by the thickness of the article.
2, since the residual stress generated by molding conditions
3, the residual stress generated when stripping
4, due to insufficient cooling time caused by the deformation

Two. The associated knowledge
1. Reasons product deformation (warping, bending, small wrinkles) with the same cracks. I.e., residual stress within the article. Molding conditions should be set towards the elimination of internal stress setting products. That increase after the cylinder temperature, mold temperature, the flowability of the material in good condition, the injection pressure is not too high.
2, in order to reduce residual stress, there is annealed, i.e., below the thermal deformation temperature of 10 degrees, there was heated over 2 hours to eliminate the effect of internal stress. Annealing in this manner but the high cost due to the use of less common.
3, if the cooling water hole of the mold can not be uniform cooling products, will produce residual stress, which means that the cooling water hole not too light.

Third, the solution.
1, real-time: in the mold sufficiently cooled and solidified (prolonged cooling time timer) enhance barrel temperature, lower injection pressure.
2. Short-term: the mold cooling uniform.
3. Long-term: to avoid differences in thickness of the article to set the thickness of the gate in products where large (1-1), because the straight line is easy to cause warping, made a large R curve, reversible bending mold products, increase the ejection lever months the number increased stripping slope.

Fourth, the material differences:

1, crystalline materials (polyethylene, polypropylene, POM, nylon) Molding shrinkage, and prone to bias, non-crystalline materials (polystyrene, ABS) likely to cause residual stresses.

2015年5月29日星期五

Injection Warpage Cause Analysis

Injection products deformation, bending, twisting phenomenon occurs mainly due to the plastic molding shrinkage flow direction than in the vertical direction is large, so that different parts of each to shrinkage and warping, and because Injection Molding unavoidable in the system the inner member has a larger residual stress caused by warping, distortion performance of these are caused by high stress orientation. So fundamentally, plastic materials mold design determines the tendency to warp parts of, to come to suppress this tendency is very difficult by changing the molding conditions, a final settlement must be designed and modified to proceed from the mold.
 This phenomenon is mainly caused by the following aspects:
1. Molds plastic materials products:
(1) The thickness of the workpiece, the quality should be uniform.
(2) The cooling system is designed to make the various parts of the mold cavity temperature uniformity, symmetry gating system to make the stream flow direction to avoid shrinkage caused by different warp, appropriate bold difficult forming part of the shunt, the mainstream road, try to eliminate the cavity density difference, pressure difference, temperature difference.
(3) the part of the transition zone thickness and angle sufficiently smooth, a good release properties, such as increased stripping redundancy, improve mold surface polishing, the top of the system to maintain balance.
(4) to the exhaust well.
(5) increase the part thickness or increase anti-warp direction, the ribs to enhance the ability of anti-warp articles.
(6) Mold materials used less rigid.

2. Plastic: the warpage opportunity crystalline appeared more than a non-crystalline plastics, combined with crystalline plastics can take advantage of the cooling rate increases with the degree of crystallinity and reduced shrinkage smaller crystallization process to correct warpage.

 3. Plastics processing:
(1) injection pressure is too high, too long dwell time, melt processing temperature is too low too fast can cause increased stress occurs warpage.
(2) mold temperature is too high, the cooling time is too short, so that parts overheat when releasing the emergence of the top of the deformation.
(3) reduction in screw speed to maintain a minimum backpressure charge quantity under reduced density and to limit the generation of internal stress.

Treatment for back-meter (4) can easily mold warpage parts soft amorphous or stripping if necessary

2015年5月27日星期三

Parts (ABS plus copper insert) cracking existential analysis and improvement

Plastic parts Name: raw materials: Terluran & reg; GP-22 type ABS + high concentration of black masterbatch problem: plastic parts intact when out of the mold in the air for 2 to 3 days, have vertical section surrounding parts of the copper insert crack, some have even been completely split. Reason analysis and improvement program: plastic parts do not have any problem during the molding process, the problem does not lie in molding equipment and technology, according to our understanding of the analysis, the problem is caused by environmental stress cracking. Cause environmental stress cracking might have the following areas:

First, the raw materials
(1) raw materials mixed with other impurities or doped with inappropriate or excessive solvents or other additives. Environmental stress cracking is a unique phenomenon polyolefin plastic, which refers to the product when there is stress, and some active media exposure, there will be a brittle crack, crack growth resulting in product damage. Such active substances may be detergents, soaps, water, oil, acids, alkalis, salts and no significant swelling effect of organic solvent materials. A necessary condition for environmental stress cracking is a pattern or part of memory in stress and stress concentration factors such as the existence of a gap, surface scratches and so on. The ABS contains a polyolefin component, and impurities contained in the starting material or solvent indirectly provides these active substances, when the ABS plastics during storage due to the emergence of a variety of causal factors surface chipped or scratched, so there will be cracks .
(2) Some plastics such as ABS, etc., in the damp heat condition can occur with moisture catalytic cracking reaction, the occurrence of large parts of the strain thus cracking.
(3) plastic barrel heating time is too long will cause brittle parts.

Second, product design

Such as polystyrene and plastic containing this ingredient as little as possible because the metal insert, because these plastic brittle cold specific volume. If the order to assemble and strength requirements must be added inserts, as inserts made of metal copper, while copper insert cooling dimensional change with heat-shrinkable plastic ABS values ​​vary greatly, resulting in a greater around the insert within stress, thus resulting in cracking products. Specific improvements are as follows:
(1) Replace the insert of the materials used to make the insert and the ABS product line expansion coefficient should be as close as possible;
(2) increase the insert sharp parts of each fillet, fillet products may cause stress concentration is too small, resulting in product cracking;
(3) increase the thickness of the insert around the plastic layer.

Third, preheat aspects inserts


With inserts in plastic products, around the insert easily crack or cause product strength decline, which is made of metal and plastic inserts for thermal and shrinkage caused by large differences. Therefore, in designing parts, should increase the wall thickness around the insert, in order to overcome this difficulty, preheated before molding is an effective measure to carry out metal inserts. Because the temperature difference between the warm-up can reduce the melt and insert in molding can melt cooling inserts around slowly, more uniform shrinkage occurs some hot material feeding action to prevent exerted around the insert large internal stress. Fourth, since the annealing processing plasticized plastic in the cylinder uneven or different cooling rate in the mold cavity, so often produce uneven crystal orientation and contraction, resulting in product there internal stress, which produces thick-walled or tape more pronounced when metal inserts products. There are parts of internal stress occurs in the storage and use of the Central Standing Committee mechanical performance, optical performance deterioration, surface crazing, cracking or deformation. Production of solving these problems is the power of a law article annealing. The method of the article is annealed in the constant temperature liquid heating medium (e.g. hot water, hot mineral oil, glycerin, ethylene glycol, and liquid paraffin, etc.) or a hot-air circulating oven was allowed to stand for some time. For ABS plastic parts plus insert, refer to the following: annealing treatment medium: water annealing temperature: 10 ~ 20 ℃ low i.e. 60 ~ 70 ℃ annealed heat distortion temperature than ABS time (85 ~ 100 ℃): 2 hours

Plastics Cracking Analysis and Countermeasures

Summary
Abstract: The cracking plastic products often fatal flaw; cracking, including filamentous workpiece surface cracks, crazing, top white, sticky parts due to cracking and mold, stick-runner or trauma caused by the crisis, by cracking time points cracking cracking and stripping applications. Causes cracking aspect relates to a mold, molding process, plastic material or the like. This paper discusses the cracking of the plastic material selection angle.

Keyword
Keywords: plastic material selection plastic cracking hot ductility balance
1: Summary of plastics defect
Plastics can be divided into external manifestation of defects defects (such as appearance, size, etc.) and internal defects (such as cracks, brittleness, etc.). The nature of the causes of defects of plastic products can be summarized as P (power), V (fill volume), T (temperature). The ultimate cause of plastic cracking is due to P (power) caused.
2: plastic cracking
Stripping cracking: plastic product from the mold stripping out or cracking in the machining process; the causes and consequences of this cracking to produce relatively easy to estimate. Applications cracking: cracking plastic products appear in the post-period of time or use. This cracking is often more difficult to predict, the consequences can be fatal. As some time before the emergence of 3G iPhone Mobile white version cover cracking phenomenon for Apple to bring in big trouble. (Battery heating up the plastic cover cause thermal expansion and contraction caused by uneven)
3: Cracking products analysis
   Whatever plastics, eventually cracking because of the nature of the force (internal stress, external force, etc.) caused. Thus we must better understand the source of power. Currently some customers some errors in the plastic of choice, resulting in a large number of plastic cracking. Now some typical case analysis

4: plastic plastic cracking prevent cracking prevention


Ways to improve the plastic cracking foreign counterparts summed up a lot of valuable experience, now from plastic material selection point of view to explore how to effectively solve the plastic cracking. In terms of product selection, we should take full account of the way the plastic molding material, component structure, heat transfer and other operational issues the actual process; for some hollow structure, should take full account of the thickness, size and so hollow. Such as thin-walled, large hollow core member should try to use good ductility (elongation at break), good thermal conductivity of plastic, and use plastic rods processed into plastic pipe will have to fully take into account the heat balance, as far as possible choose ductile plastic rods, for some ductility bad plastic pipe, as far as possible avoid using bar processed into pipe (pipe general factory has been heat-treated residual stress). For some ductility bad plastic, plastic pipes and plastic rod effect is not the same. Cracking satisfy the conditions: μl / hßΨ≥ ξ μ- empirical process factor, h- wall thickness, l- hollow perimeter, ß- plastic shrinkage, Ψ- plastic thermal conductivity, ξ- breaking elongation 5. Conclusion prevent cracking of the most difficult point of plastic products is how to prevent the plastic products in different parts of the apparent thermal equilibrium, and the use of carbon fiber or metal filled plastic, because the strong heat conduction capability, so a relatively small chance of cracking. From the viewpoint of a plastic material, products related to cracking the wall thickness, volume hollow products, plastic ductility.

2015年5月21日星期四

The plastic parts aberration control

Products color is common defects in injection molding, because the accessories and aberration caused by injection molding machine, does not see small batch scrap. Aberration affected by many factors, involving raw materials for resin, pigment, pigment mixed with raw materials, such as injection molding process, injection molding machine, mold, and because of the impact is widespread, so the aberration control technology is also one of recognized difficult to master the technology of injection molding. The actual production process we generally from the following six aspects: to control the aberration.

1, to eliminate the influence of the injection molding machine and mold factors to choose with considerable injection molding machine, injection molding products for capacity if material corner problems in injection molding machine, best replacement equipment. For mould gating system, such as exhaust slot cause off color, through the corresponding part of the mould maintenance mode to solve. Must first solve the problem of good injection molding machine and mold to organize production, to reduce complexity of the problem.

2, eliminate the influence of raw material resin, color master control of raw materials is the key to thoroughly solve the aberration. Therefore, especially the production of light color products, not ignore the thermal stability of resin raw material the obvious effects of different colour and lustre of products fluctuations. Given that most of the injection molding manufacturers itself does not produce plastic masterbatch or masterbatch, such, can be the focus of attention on the production management and raw material inspection. Namely to strengthen raw material incoming inspection; As much as possible in the production of the same products using the same manufacturer, same brand masterbatch, masterbatch production. For pigment, we will try to check the color before mass production, as well as with the last time to proofread, and in the comparison, if the aberration is not big, qualified, can be thought of as has slight aberration, color master batch can be used after mixing pigment back again, in order to reduce uneven mixing pigment itself the brightness of the photo. With, we still need to focus on inspection raw material resin, pigment, the thermal stability of the poor thermal stability, we suggest that the manufacturer and exchange.

3, eliminate the influence of uneven pigment mixed with masterbatch plastic masterbatch mixed with pigment is bad also can make the product color changes. After mother and masterbatch mechanical mixing, through the absorption into the hopper, due to electrostatic interactions, masterbatch masterbatch with separation, easy adsorption in the hopper walls, and this is bound to cause injection cycle at the mother volume changes, resulting in a aberration. This kind of circumstance can take again after raw material suction hopper to artificial mixing solution. Now there are a lot of companies feed machine is used to add pigment, thereby saving a lot of manpower, and for the aberration control provides a lot of help, but many companies because of improper use, the results are often difficult to satisfactory. Join masterbatch feeding machine under fixed speed depends on plasticizing time, and plasticizing time itself is volatile, sometimes even more volatile, so to ensure the constant feed rate, the feeder must be fixed feeding time, and set a time less than the minimum plasticizing time. In the use of feeding machine need to notice, due to the feeder exports is small, use after a period of time, may be because the accumulated material used in the feeding machine screw powder caused blanking, even cause feeding machine stops, so need to regular cleaning.

4, reduce the influence of cylinder temperature on aberration in a heating coil damage failure of production often encounter or control of heating control part long fire ChengLiao tube rapid changes in temperature to produce off color. This kind of reason of aberration is easy to determine, general damage of heating coil Produce off color, but at the same time will be accompanied by plasticizing uneven phenomenon, and the heating control part is out of control long burning gas spot is often associated with products, severe discoloration even coking phenomenon. So the need to check the heating part of the production, found that the heat damage or change in time maintenance when out of control, in order to reduce this kind of aberration.

5, and reduce the influence of the injection molding process adjustment when the chromatism reason need adjust injection molding process parameters, as far as possible, don't change the molding temperature, the amount of back pressure, the injection molding cycle and masterbatch, adjust at the same time also need to observe the effects of process parameters change on colour and lustre, for example, when found aberration should be and adjustment. As far as possible avoid the use of high speed and high back pressure injection cause strong shearing action of the injection molding process, prevent due to factors such as local overheating or thermal decomposition of the brightness of the photo. Strict control of cylinder each heating section temperature, especially the nozzle and close to the heating part of the nozzle.

6, master cylinder temperature, the influence of the change of product color masterbatch quantity before color adjustments must also know the product color change with temperature, pigment volume trends. Different mother color change with the temperature of the production or the amount of pigment, the product color change law is different. Color can be through the test process to determine its change law. Unless you have know this kind of pigment color change rule, otherwise cannot be quickly adjusted the aberration, especially in the new color masterbatch production.

The judgement of plastic product aberration

When molding plastic products, its product colors and materials has a direct touch its mainly manifested in the following aspects:

1. The color relations with incoming plastic granule. Due to the product raw material plastic material batch change frequently, and each batch of raw material Material, were inconsistent aberration phenomenon, such as some incoming slant blue color, has the processing slant red color, and so on, so we in the acceptance of incoming (sample) must sample product contrast aberration with customer's original sample and luster. Only in color and luster completely in line with and without other problems when the material can be thought of as good.

Relationship. 2. The color and material tube temperature used material aberration with the feed tube temperature relationship which were as follows; Feed tube at the higher temperature, a partial value red color, b value big yellow, L value little darker. But there are also in the process of forming phase for special case, so in molding should also to match the die temperature in debugging off color problem. Mould temperature, the higher the L value into negative dimmed, a, b.


3 colors and material drying temperature care generally speaking, the color and material drying temperature also has relatively direct contact: such as PC/PA transparent material, drying temperature too high and the time is too long, the color will be become yellow or black, forming the product transparency. Such as ABS material, drying temperature too high or too long, will lead to poor products change yellow and sex. We in front of the molding products must be in 3 to 4 hours before starting the preliminary drying to dry materials will be not too long time and too high temperature baking, so as to avoid product color run, as a result of product aberration And bad. But when molding material tube temperature is too high there will be some phase should be quality problem,, such as product performance, product package (poor exhaust) wind and so on. So I have aberration when molding products mainly come from raw materials incoming problem, method of control can only play an auxiliary role.

2015年5月15日星期五

Problem Cause incomplete filling of plastic products and solutions

A meaning: after the melt into the mold cavity does not fill completely, causing plastic parts shortage of material.

Second, Causes and Remedy:

①, improper selection of equipment: When sorting equipment, melt glue machine must be greater than the amount of molten plastic products, plastic parts by weight of the machine can only account for 85% of the total amount of melt.

②, feed shortage: the charging port if there is "bridging" phenomenon, may be appropriate to increase the screw injection stroke, increasing the feed rate.

③, raw illiquid: improved die casting system stagnation defect, a reasonable set of pouring glue position, expanding gates, runners and injection spout sizes and use larger nozzle, an appropriate increase in raw material temperature.

④, gating system design is unreasonable: gating system design, pay attention to the gate balance, the weight of the plastic parts of each cavity is proportional to the gate, the cavities are filled simultaneously, gate locations to be selected in the original wall parts, sub-runner balance design layout can also be used.

⑤, mold exhaust bad: check cold material cavity, or location is correct, for deep cavity mold, should be added to the exhaust vent in the trenches and less injection site, the clamping surfaces can be opened Deep 0.02 -0.04mm, 5-11mm in width exhaust ducts, vents should be provided in the final filling of the mold cavity. Also in the process of operation, by increasing the die temperature, reducing the injection speed, gating system to reduce resistance, and to reduce the clamping force.

⑥, mold temperature is too low: the mold must be preheated to the required temperature before starting the process, if the mold temperature does not rise up, check the mold design is not only reasonable waterway.


⑦, the injection pressure is insufficient: the length of the injection pressure is close to a positive relationship with the die, injection pressure is too small, short filling length, filling the cavity dissatisfaction, which can slow down the plunger forward speed through proper injection ting long time to improve injection pressure.